What it is

Kind
Fluxes
Formula
CaO•SiO₂ (ideal CaSiO₃: CaO 48.28, SiO₂ 51.72)
Also called
NYAD 400, NYAD, Wollastonite NYAD, NYAD-G, NYAD 325, NYAD M200
Made by
NYCO Minerals, Willsboro, New York (now part of Imerys)
Sold in
US
Source
NYCO data sheet 'Wollastonite NYAD 400' (document IN-071-05-2, undated) (2012-07)

High-purity New York wollastonite with low LOI. Imerys markets NYAD M200, M325 and M400 grades for ceramic bodies and glazes; Sheffield Pottery sells NYAD-G.

Oxide analysis and unity formula

Glazecalc has the analysis of Wollastonite (NYAD 400) as weight percent of the raw material. The unity contribution is the moles of each oxide in the amount of Wollastonite (NYAD 400) that holds 1.0 mole of flux, which is how Glazecalc adds it into a recipe's unity formula.

Oxides in Wollastonite (NYAD 400)
Oxide Weight % Unity contribution
CaO46.360.993
SiO₂51.61.031
Fe₂O₃0.770.006
Al₂O₃0.40.005
MnO0.150.003
MgO0.150.004
TiO₂0.050.001
K₂O0.020.000
Equivalent weight
120.08
Fired weight
119.48
Loss on ignition
0.5%

The equivalent weight is the grams of Wollastonite (NYAD 400) that hold 1.0 mole of flux. The fired weight is what is left of that after firing.

Hazards and safety

Hazards: Needle-shaped (acicular) mineral dust; avoid breathing it.

Glazecalc shows the hazard wording as its record gives it. It is not a full risk assessment, so read the safety data sheet from your supplier. Before you handle any glaze material, read Safe mixing and ventilation and Glaze safety at home.

Use it in a recipe

Add Wollastonite (NYAD 400) to a recipe in the Glazecalc calculator to see what it does to a glaze's unity formula.